Sample: Mg-3Al_5p0 Ungroup Processes
Last Updated: 2 days ago Owner: Tracy Berman ID: 67405
EPMA Data Collection (8)
Date:
42655
Date:
42368
Date:
42359
Date:
42293
Region of interest:
near edge
Region of interest:
center
Region of interest:
edge
Elements Measured:
Mg, Al, Zn, Mn
Elements Measured:
Al, Mg
number of measurements made:
400
data start row:
901
data start row:
1201
data start row:
1601
data start row:
2001
data start row:
1301
data end row:
1300
data end row:
2000
data end row:
2400
data end row:
1700
data end row:
1600
Measurements
Alloy Name:
Mg-3Al
beta + Al-Mn phase fraction:
0.866 %
beta + Al-Mn phase fraction:
0.393 %
beta + Al-Mn phase fraction:
1.008 %
Mean experimental Al content:
1.18 wt%
Mean experimental Al content:
3.11 wt%
Mean experimental Al content:
3.14 wt%
Plate Thickness:
5 mm
Standard deviation:
0.159 %
Standard deviation:
0.127 %
Standard deviation:
0.219 %
Composition Al Content:
3.12 wt %
Composition Mn Content:
0.09 wt %
Composition Mg Content:
96.79 wt %
Files
EPMA WIRS Analysis (3)
Date:
10/26/2016
Region of Interest:
Edge
Region of Interest:
Near Edge
Region of Interest:
Center
Measurements
Alloy Name:
Mg-3Al
beta + Al-Mn phase fraction:
0.866 %
beta + Al-Mn phase fraction:
1.008 %
beta + Al-Mn phase fraction:
0.393 %
Mean experimental Al content:
3.14 wt%
Mean experimental Al content:
3.11 wt%
Mean experimental Al content:
1.18 wt%
Plate Thickness:
5 mm
Standard deviation:
0.219 %
Standard deviation:
0.127 %
Standard deviation:
0.159 %
Composition Al Content:
3.12 wt %
Composition Mn Content:
0.09 wt %
Composition Mg Content:
96.79 wt %
Files
Forward Model Simulation (12)
Region of Interest:
center
Region of Interest:
edge
Region of Interest:
near edge
Simulated partition coefficient:
0.3 k_v
Simulated partition coefficient:
0.25 k_v
Simulated partition coefficient:
0.35 k_v
Simulated partition coefficient:
0.4 k_v
Simulated partition coefficient:
0.45 k_v
Simulated partition coefficient:
0.5 k_v
Simulated partition coefficient:
0.55 k_v
Mean simulated Al contentl:
2.86 wt%
Mean simulated Al contentl:
2.71 wt%
Mean simulated Al contentl:
3.16 wt%
Mean simulated Al contentl:
2.99 wt%
Mean simulated Al contentl:
2.58 wt%
Mean simulated Al contentl:
2.82 wt%
Mean simulated Al contentl:
2.85 wt%
Mean simulated Al contentl:
2.45 wt%
Mean simulated Al contentl:
3.01 wt%
Mean simulated Al contentl:
1.29 wt%
Mean simulated Al contentl:
3.04 wt%
Mean simulated Al contentl:
1.17 wt%
Least Squares difference simulation versus experiment:
0.39
Least Squares difference simulation versus experiment:
0.3
Least Squares difference simulation versus experiment:
0.06
Least Squares difference simulation versus experiment:
0.27
Least Squares difference simulation versus experiment:
0.09
Least Squares difference simulation versus experiment:
0.17
Least Squares difference simulation versus experiment:
0.25
Least Squares difference simulation versus experiment:
0.03
Least Squares difference simulation versus experiment:
0.37
Least Squares difference simulation versus experiment:
0.52
Measurements
Alloy Name:
Mg-3Al
beta + Al-Mn phase fraction:
0.393 %
beta + Al-Mn phase fraction:
0.866 %
beta + Al-Mn phase fraction:
1.008 %
Mean experimental Al content:
3.14 wt%
Mean experimental Al content:
3.11 wt%
Mean experimental Al content:
1.18 wt%
Plate Thickness:
5 mm
Standard deviation:
0.159 %
Standard deviation:
0.127 %
Standard deviation:
0.219 %
Composition Al Content:
3.12 wt %
Composition Mn Content:
0.09 wt %
Composition Mg Content:
96.79 wt %
Files
Phase Fraction Analysis (3)
Region of Interest:
Near Edge
Region of Interest:
Edge
Region of Interest:
Center
Number of images analyzed:
10
Measurements
Alloy Name:
Mg-3Al
beta + Al-Mn phase fraction:
0.393 %
beta + Al-Mn phase fraction:
1.008 %
beta + Al-Mn phase fraction:
0.866 %
Mean experimental Al content:
1.18 wt%
Mean experimental Al content:
3.11 wt%
Mean experimental Al content:
3.14 wt%
Plate Thickness:
5 mm
Standard deviation:
0.159 %
Standard deviation:
0.127 %
Standard deviation:
0.219 %
Composition Al Content:
3.12 wt %
Composition Mn Content:
0.09 wt %
Composition Mg Content:
96.79 wt %
Files
Received As-Cast Plates (1)
Measurements
Alloy Name:
Mg-3Al
beta + Al-Mn phase fraction:
0.393 %
beta + Al-Mn phase fraction:
1.008 %
beta + Al-Mn phase fraction:
0.866 %
Mean experimental Al content:
3.14 wt%
Mean experimental Al content:
3.11 wt%
Mean experimental Al content:
1.18 wt%
Plate Thickness:
5 mm
Standard deviation:
0.127 %
Standard deviation:
0.219 %
Standard deviation:
0.159 %
Composition Al Content:
3.12 wt %
Composition Mn Content:
0.09 wt %
Composition Mg Content:
96.79 wt %
SEM Imaging (3)
Date:
3/14/2016
Region of Interest:
Center
Region of Interest:
Edge
Region of Interest:
Near Edge
View Field Width:
50 µm
View Field Width:
200 µm
Imaging Mode:
SE
Voltage:
10 keV
Beam Intensity:
10
Measurements
Alloy Name:
Mg-3Al
beta + Al-Mn phase fraction:
0.393 %
beta + Al-Mn phase fraction:
1.008 %
beta + Al-Mn phase fraction:
0.866 %
Mean experimental Al content:
1.18 wt%
Mean experimental Al content:
3.11 wt%
Mean experimental Al content:
3.14 wt%
Plate Thickness:
5 mm
Standard deviation:
0.219 %
Standard deviation:
0.127 %
Standard deviation:
0.159 %
Composition Al Content:
3.12 wt %
Composition Mn Content:
0.09 wt %
Composition Mg Content:
96.79 wt %
Files