Sample: ZX0p50_d51 Ungroup Processes
Last Updated: 2 days ago Owner: Tracy Berman ID: 67491
Gleeble (1)
Test date:
8/30/2021
Start Thickness:
10 mm
Final Thickness:
1.95 mm
Deformations:
10
Program Strain Type:
TRUE
Pre-deformation Soak Temp:
350 ºC
Rate to Temp:
5 ºC/s
Pre-deformation Soak Time:
600 s
Initial Strain Rate:
0.5 /s
Strain Per pass:
0.2
Stage One - Temp during Deformations:
350 ºC
Stage One - interpass anneal Temp:
350 ºC
Stage One - interpass anneal Time:
600 s
Stage Two - Number of passes:
0
Quench Duration:
30 s
Measurements
Alloy:
ZX0p50
Composition Zn content:
0.5 wt%
Composition Ca content:
0.1 wt%
Files
Receive Samples (1)
Receipt Date:
11/2/2018
Source:
University of Florida
Measurements
Alloy:
ZX0p50
Composition Zn content:
0.5 wt%
Composition Ca content:
0.1 wt%
Files